When it works above 180 degree temperature, its magnetic power and reliability are better than the NdFeB magnet. It is a bit lower magnetic power than NdFeB magnet, but it need to no electroplating. Because it has wide using range, it is applied in aerosol products, the concise machines and high-technology areas.

   
Magnetic Characteristics & other physical characteristics of Sinter SmCo Magnets

SmCo Magnet

Grade

Residual induction

Intrinsic Coercive

Coercive Force

Max.Energy Product

Curie

Br

Hcj

Hcb

(BH)max

Temp.( O C)

MT

KG

KA/m

KOe

KA/m

KOe

KJ/m3

MGOe

SmCo5

ESC-18

850-900

8.50-9.00

1194-1513

15-19

620-648

7.80-8.20

127-143

16-18

750

ESC-20

920-960

9.20-9.60

1194-1513

15-19

653-717

8.20-9.00

150-167

19-21

750

ESC-24

960-1000

9.60-10.20

1194-1513

15-19

730-770

9.20-9.70

175-190

22-24

750

SmCo17

ESC-G24

950-1020

9.50-10.20

1433-1990

18-25

637-732

8.00-9.20

175-190

22-24

800

ESC-G26

1020-1050

10.20-10.50

1433-1990

18-25

748-796

9.40-10.0

195-215

24-26

800

ESC-G28

1050-1080

10.50-10.80

1433-1831

18-25

756-796

9.50-10.0

205-220

26-28

800

ESC-G28B

1020-1100

10.20-11.00

440-520

5.5-6.5

420

5.20-5.60

205-220

26-28

800

ESC-G30

1080-1100

10.80-11.00

955-1195

18-25

780

9.80-10.5

220-240

28-30

800

ESC-G30B

1080-1150

10.80-1150

440-520

5.5-6.5

420

5.20-5.60

220-240

28-30

800